Need help: Bizarre Bravo III freshwater galvanic corrosion quandry

cyclops222

Captain
Joined
Mar 21, 2024
Messages
3,218
Luck beats skill every time in a problem like this.
Big marinas with power outlets in use ??
 

Cdn20valve

Seaman
Joined
Aug 10, 2015
Messages
55
It was my understanding that using mercathode and having magnesium anodes cancel each other out by both over protecting. While using mercathode, you need to use aluminum anodes. This might be the source of your problem.
 
Last edited:

alldodge

Moderator
Staff member
Joined
Mar 8, 2009
Messages
44,673
It was my understanding that using mercathode and having magnesium anodes cancel each other out by both over protecting. While using mercathode, you need to use aluminum anodes. This might be the source of your problem.
Not correct, different metals have different properties and do effect current
 

paulswagelock

Petty Officer 2nd Class
Joined
Jan 10, 2018
Messages
106
Do you have a galvanic isolator installed? You should.
if you have a pro sport charger, you can ground the chassis of the charger. Talk to their tech support, there was a known issue where that charger could contribute to the problem.
 

drewm3i

Petty Officer 1st Class
Thread starter
Joined
Dec 31, 1969
Messages
328
I'm an ABYC-certified corrosion technician, and here are my two cents....

You need to get a silver/silver chloride reference cell and throw it overboard and see what you get for readings. Anything other than that is guessing at things. If your anodes are NOT corroding, that would point to electrolytic corrosion. With electrolytic corrosion, the cathode corrodes, not the anode.
With a reference cell connected to your multimeter's negative input, and the meter's positive lead connected to battery ground, you should get -800 to -1100 millivolts DC with all electrical systems off, including the mercathode.
  • If you are a high, you have cathodic corrosion going on, which means that your boat may have too many anodes, the wrong type of anodes, or a boat next to yours has too many anodes or the wrong type.
  • If you are low, that is galvanic corrosion, which means too few anodes, the wrong type of anodes, or a boat or structure near your boat has a lot of underwater stainless steel that your boat needs to account for.
Next, start turning on items 1 at a time and see if the reading changes. The readings should not change. If the readings change, especially a shift from - to +, there is DC stray current in the water coming from whatever is being turned on. The common offenders are trim senders, trim limits switches, faulty mercathode, and faulty bilge pump.
Good advice, but I'm like 99% sure I solved this. Keep in mind this was not "my slip," but transient ones that we were at for like four nights at one place and five at another. This boat is not, nor has ever been, slipped beyond a few days. The corrosion was never present in salt or brackish water because it is more conductive than fresh.

Even with stray AC current, the only logical cause was the loose 12VDC trim sender wires that were powered until I disconnected them from the engine harness recently.

Also, the anodes are indeed corroding/pitting, but just doing so very slowly; but that is to be expected in the cold, crystal clear Great Lakes water for a trailer queen. The anodes are also essentially brand new--as is the Mercathode and bonding system--so...

I think this whole thread, it turned out, was much ado about nothing since the obvious culprit were the cut/mangled trim sender wires which were essentially touching the gimbal ring with 12 volts DC anytime the key was in the "on" position...
 

drewm3i

Petty Officer 1st Class
Thread starter
Joined
Dec 31, 1969
Messages
328
Do you have a galvanic isolator installed? You should.
if you have a pro sport charger, you can ground the chassis of the charger. Talk to their tech support, there was a known issue where that charger could contribute to the problem.
I don't have one, nor do I have a shorepower system--just the charger. The chassis is indeed grounded per the manufacturer's specifications.
 

Scott06

Fleet Admiral
Joined
Apr 20, 2014
Messages
7,628
Good advice, but I'm like 99% sure I solved this. Keep in mind this was not "my slip," but transient ones that we were at for like four nights at one place and five at another. This boat is not, nor has ever been, slipped beyond a few days. The corrosion was never present in salt or brackish water because it is more conductive than fresh.

Even with stray AC current, the only logical cause was the loose 12VDC trim sender wires that were powered until I disconnected them from the engine harness recently.

Also, the anodes are indeed corroding/pitting, but just doing so very slowly; but that is to be expected in the cold, crystal clear Great Lakes water for a trailer queen. The anodes are also essentially brand new--as is the Mercathode and bonding system--so...

I think this whole thread, it turned out, was much ado about nothing since the obvious culprit were the cut/mangled trim sender wires which were essentially touching the gimbal ring with 12 volts DC anytime the key was in the "on" position...
delete
 

JustJason

Vice Admiral
Joined
Aug 27, 2007
Messages
5,394
Good advice, but I'm like 99% sure I solved this. Keep in mind this was not "my slip," but transient ones that we were at for like four nights at one place and five at another. This boat is not, nor has ever been, slipped beyond a few days. The corrosion was never present in salt or brackish water because it is more conductive than fresh.

Even with stray AC current, the only logical cause was the loose 12VDC trim sender wires that were powered until I disconnected them from the engine harness recently.

Also, the anodes are indeed corroding/pitting, but just doing so very slowly; but that is to be expected in the cold, crystal clear Great Lakes water for a trailer queen. The anodes are also essentially brand new--as is the Mercathode and bonding system--so...

I think this whole thread, it turned out, was much ado about nothing since the obvious culprit were the cut/mangled trim sender wires which were essentially touching the gimbal ring with 12 volts DC anytime the key was in the "on" position...
Happy to hear you figured it out. BTW, for all intents and purposes, AC stray current is generally not an issue for electrolytic corrosion in the marine enviorment. While AC stray current can cause electrolytic corrosion, it takes AC stray current a year to cause the same corrosion damage that DC can do in a day.
 

drewm3i

Petty Officer 1st Class
Thread starter
Joined
Dec 31, 1969
Messages
328
Happy to hear you figured it out. BTW, for all intents and purposes, AC stray current is generally not an issue for electrolytic corrosion in the marine enviorment. While AC stray current can cause electrolytic corrosion, it takes AC stray current a year to cause the same corrosion damage that DC can do in a day.
I appreciate you taking the time to share your knowledge with us! Piecing the puzzle together, it is clear that those powered trim sender wires are a clear corrosive hazard. @tpenfield had a similar corrosion issue and also had trim sender wires in the water judging from the pictures.
 

tpenfield

Moderator
Staff member
Joined
Jul 18, 2011
Messages
19,599
I've always considered the trim (and trim limit) senders a bad design, since that electrical stuff is below the water line, and the associated movement of the outdrive promotes fraying of the wires.

Hopefully, you've got it sorted out now.

Are you going to keep the Chappy? Did you buy the sailboat that you were considering?
 

JustJason

Vice Admiral
Joined
Aug 27, 2007
Messages
5,394
I appreciate you taking the time to share your knowledge with us! Piecing the puzzle together, it is clear that those powered trim sender wires are a clear corrosive hazard. @tpenfield had a similar corrosion issue and also had trim sender wires in the water judging from the pictures.
You are very welcome.
 

Lou C

Supreme Mariner
Joined
Nov 10, 2002
Messages
14,537
Agreed and if the sending unit lasts more than 2 seasons it's a surprise, I lost track of how many times I've replaced it. At least 4.
 
Top